Standard TPU (90A–98A) print settings

By Tony Tate · updated 2026-11-27 · First Layer 1.0.2

Standard TPU (90A–98A) prints at about 225 °C with a 45 °C bed and 30% part cooling. Usable range 210–240 °C nozzle, 25–60 °C bed. No enclosure needed.

TPU 95ATPU 98ATPU 90AFlexibleThermoplastic PolyurethaneMedium TPU

Starting settings

starting points Every number here is drawn from manufacturer data sheets across the material as a whole. None of it is a measurement of the spool in your hand, and brand-to-brand variation inside one material is wider than most people expect. Where a figure says "about", the app holds one typical value rather than a range. Treat all of it as somewhere to begin, then measure — shrinkage and flow especially, because those two are what throw dimensions off.

Nozzle
210–240 °C (start 225)
Bed
25–60 °C (start 45)
Part fan
0–50% (start 30%)
Wall speed
10–30 mm/s
Max volumetric flow
about 3.5 mm³/s
Shrinkage
about 0.6%
Glass transition
about -35 °C — flexible above it, so at room temperature it is rubbery rather than soft
Enclosure
Not needed
Nozzle size
0.4 mm or larger — 0.4 mm recommended
Nozzle material
Brass is fine
Drying
about 50 °C for 6 h

Speed

MUCH SLOWER — 10–30 mm/s, and this is the single most important setting on this material. Above roughly 30 mm/s the filament buckles in the drive gear instead of feeding, and no other change fixes it.

Bed surface

Clean smooth PEI, no adhesive needed — TPU grips well on its own at 45 °C.

Nozzle

0.4 mm is fine. A larger nozzle helps, since flexible filament resists being forced through a small opening.

What bites people

Safety

Common questions

What temperature should I print Standard TPU (90A–98A) at?

Start at 225 °C nozzle and 45 °C bed, within a usable range of 210–240 °C and 25–60 °C. Run a temperature tower on your own spool rather than trusting any table: brand-to-brand variation inside one material is wider than most beginners expect.

Does Standard TPU (90A–98A) need an enclosure?

No. Standard TPU (90A–98A) prints fine on an open-frame machine.

What nozzle do I need for Standard TPU (90A–98A)?

0.4 mm or larger, with 0.4 mm recommended. A brass nozzle is fine.

Open First Layer →
The app walks this in order, generates the test model for your nozzle and filament, and records what you measure so nothing has to be repeated. Free, no account, works offline.